148
Gas Tungsten Arc Welding Handbook
Melt-through. Occurs at a gap in the weld joint or place where metal is thin.
How to correct:
Decrease current.
Increase arc length.
Increase travel speed.
Decrease root opening.
Concave root surface. The root of the weld penetration does not extend below the lower edges of the joint.
How to correct:
Decrease travel speed.
Decrease amperage.
Decrease arc length.
Increase fi ller wire deposition.
Icicles. Weld penetration beyond the joint root is uneven.
How to correct:
Move the torch throughout the weld length
in a consistent pattern.
Add fi ller metal as required to maintain an
even penetration.
Previous Page Next Page